The lamination stack is the magnetic backbone of every motor. The steel grade sets the iron loss; the stamping and stacking quality decides whether you actually get that low loss in the finished motor.
1. Introduction
A motor core is not one solid block of iron. It is hundreds of thin, insulated sheets of electrical steel stacked together. When a designer specifies "M400-50A" and the stack comes with high burrs, shorted sheets or a loose stack, the motor fails its efficiency test even though the design was right. This blog explains the grades, the loss, and the process from coil to core.
2. Why laminate at all?
The magnetic field in a motor core changes direction 50 times a second (and much faster in BLDC and EV motors). A changing field induces circulating eddy currents inside the steel, which heat it. Thin sheets with an insulating coating cut these current paths. A second loss, hysteresis loss, comes from re-magnetising the steel every cycle; it is reduced by adding silicon and by good annealing. Together they are called core loss or iron loss, measured in W/kg.
3. Electrical steel grades (EN 10106, non-oriented)
The grade name tells you the loss: M400-50A = maximum 4.00 W/kg at 1.5 T, 50 Hz, thickness 0.50 mm, "A" = fully processed non-oriented. Motors use non-oriented (CRNO) steel because flux turns in all directions; transformers use grain-oriented (CRGO).
| Grade | Thickness (mm) | Max core loss at 1.5 T, 50 Hz (W/kg) | Typical use |
|---|---|---|---|
| M235-35A | 0.35 | 2.35 | Premium efficiency, high-speed and EV motors |
| M250-35A | 0.35 | 2.50 | IE3/IE4 motors, BLDC, compressors |
| M270-35A | 0.35 | 2.70 | High-efficiency motors |
| M300-35A | 0.35 | 3.00 | Efficient medium motors |
| M250-50A | 0.50 | 2.50 | High-efficiency, lower punching cost than 0.35 |
| M400-50A | 0.50 | 4.00 | General-purpose industrial motors |
| M470-50A | 0.50 | 4.70 | Standard motors, pumps |
| M530-50A | 0.50 | 5.30 | Cost-focused motors |
| M800-50A | 0.50 | 8.00 | Fans, appliances, low-cost motors |
The trade-off: lower-loss grades have more silicon, so they are slightly lower in saturation flux density, harder to punch (more die wear) and cost more. Higher-loss grades are more permeable and cheaper.
4. From steel coil to core – the process
- Slitting the mother coil to the strip width needed for the die.
- Stamping in a high-speed press with a progressive die (slot notching, rotor and stator blanking in stations) or compound die. Rotor and stator are often punched from the same strip to save material.
- Stacking – laminations are joined into a core by one of the methods below.
- Optional stress-relief annealing for semi-processed steel or to recover loss after punching.
- Inspection – burr height, ID/OD, slot dimensions, stack height, squareness, stack weight, and core-loss test on samples.
| Stacking method | How it works | Good points | Watch-outs |
|---|---|---|---|
| Interlocking (auto-stack in die) | Small dimples press into the next sheet inside the die | Fast, no extra station, used for most mass-production cores | Small local loss at interlock points; stack can loosen if dimple depth is wrong |
| Welding (TIG/laser) | Weld seams along the stack OD | Strong, rigid | Weld shorts sheets together and raises loss; heat stress |
| Bonding (adhesive / self-bonding coating) | Glue dots or bonding varnish join every sheet | Lowest loss, low noise, no shorts | Slower, curing time, higher cost |
| Riveting / cleating | Rivets or clips through/around the stack | Simple for large or low-volume cores | Rivets may create loss paths; extra parts |
5. Key quality parameters
| Parameter | Why it matters | Typical control |
|---|---|---|
| Burr height | Burrs pierce coating and short sheets, raising eddy loss | Keep very low (often within a few hundredths of a mm); regrind die on schedule |
| Stacking factor | Steel fraction of stack height | About 0.95–0.97 for good flat steel |
| Slot dimensions and position | Coil insertion, slot fill, air gap uniformity | Die accuracy, regular CMM checks |
| Stack height and weight | Torque and flux per motor | Count or weigh-controlled stacking |
| Squareness and concentricity | Air gap, noise, vibration | Fixtures, interlock design |
| Coating integrity | Insulation between sheets | Right coating class; avoid scratching |
6. Common problems – root cause – solution
| Problem | Root cause | Solution |
|---|---|---|
| Motor fails efficiency test, high no-load loss | Burrs shorting sheets; welding seams; punching stress | Die sharpening schedule; switch to interlock or bonding; stress-relief anneal |
| Loose stack, noise | Interlock depth wrong; strip thickness variation | Correct interlock geometry; check incoming strip thickness |
| Coil insertion damage | Sharp slot edges, burrs at slot mouth | Deburr; correct die clearance |
| Air-gap variation | Bore not round; stack skewed | Check bore roundness; better stacking fixture |
| High die wear | Low-loss high-silicon grade is abrasive | Carbide die inserts; planned regrind |
7. Videos to watch (16)
| # | Video | Channel | Length | Why watch |
|---|---|---|---|---|
| 1 | Stator Laminations = More Power! (But Why?) | Stephan_RC | 1:48 | Quick visual of why we laminate |
| 2 | What is Eddy Current Loss & Hysteresis Loss | Electrical lectures | 3:46 | The two core losses |
| 3 | How Electric Vehicles Work – Electrical Steel | Swansea University (Materials & Manufacturing) | 19:20 | Electrical steel in depth |
| 4 | Motor Stator Core: Eddy Current Loss | Rotor Dynamics 101 | 4:52 | Loss in stator cores |
| 5 | Module 12: Stator Laminations & Core Design Studies | CUSP | 27:51 | Design lecture on cores |
| 6 | Core and Magnet Losses in Electric Motors (Ansys Maxwell) | Ozen Engineering | 5:24 | Simulating core loss |
| 7 | Stamping Press for Motor Stator and Rotor Lamination | MechTech stuff | 4:30 | Press stamping in action |
| 8 | Progressive Stamping of EV Drive Motor Cores | Lammotor | 1:26 | EV core stamping |
| 9 | Progressive Stamping and Welding EV Motor Core Laminations | Lammotor | 1:57 | Stamping plus welding |
| 10 | Compound Stamping Stator and Rotor Core Lamination | Lammotor | 1:21 | Compound die method |
| 11 | Lamination Helical Coiling Stamping Line for EV Motor | stamping die maker | 0:48 | Helical (spiral) cores |
| 12 | Motor Lamination Manufacturing: Stamping vs Laser Cutting vs Chemical Etching | Precision Micro | 1:41 | When to use which process |
| 13 | Bonding Lamination Stacks – Why Adhesive? | best-statorcore | 2:57 | Bonded cores explained |
| 14 | Robotic Welding – Stator Core Laminations | Orchid International | 1:18 | Automated stack welding |
| 15 | Auto-Interlock Stacking Die (Stator and Rotor) | Stamping Die and Deep drawing die | 2:42 | Interlock stacking in the die |
| 16 | How to Test for Core Loss in Your Motors | Industrial Electric Motor Service | 6:14 | Core loss testing |
8. Sources referred
- Electrical steel strip DIN EN 10106 – data sheet, Waelzholz (max core loss and polarisation by grade)
- Non-oriented fully processed electrical steel – Cogent/Surahammars Bruks brochure (grade table, stress and burr effects)
- Electrical steel for high-efficiency motors – Tata Steel / Surahammars Bruk
- Electrical steel grade catalogue – ArcelorMittal (EN / AISI / JIS equivalents)
- EN 10106 Grade M400-50A – property sheet (stacking factor 0.96)
Share your experience. Have winding data, a shop-floor photo or a doubt on this topic? Join the MotorMakers India community and help others learn.